Two condensations, one wanted and one not

Flue gas from a gas or oil boiler carries water vapour and, from a sulphur-bearing fuel, sulphur trioxide. Cooling it below the water dew point of 55-60 °C condenses water and releases recoverable latent heat. Cooling it below the acid dew point, 120-160 °C depending on the fuel, condenses sulphuric acid onto metal. The first is the basis of a condensing boiler; the second eats economisers, stack linings and fan impellers.

Both happen in the same tail-end exchanger if the design is careless. The question is not whether to condense but where, at what temperature and against what material. A boiler that condenses in a purpose-built condenser with a drain and a neutralising trap is recovering heat. A boiler that condenses in the last fin of an economiser or the top of an uninsulated stack is corroding.

Water dew point and acid dew point

The water dew point follows from the partial pressure of water vapour. Natural gas flue gas contains 15-18% water vapour, which gives a dew point of 55-60 °C. Oil flue gas is similar, and biomass flue gas is higher in moisture, often 12-20% with a dew point of 55-65 °C. Below that temperature, water condenses; the latent heat released is about 2,440 kJ per kilogram of water, and that is the heat a condensing economiser is designed to capture.

The acid dew point is higher and more damaging. Sulphur in the fuel burns to sulphur dioxide, and 1-3% of that is further oxidised to sulphur trioxide in the flame. The SO3 combines with water vapour to form sulphuric acid vapour, which condenses on surfaces below 120-160 °C. The figure depends on SO3 concentration, water vapour and pressure, and rises with sulphur content. The table gives the range for common fuels.

A second mechanism matters for biomass: hydrochloric acid from chloride in the fuel, with a dew point of 90-110 °C, and alkali chloride deposits that corrode tubes well above the water dew point. A biomass boiler can suffer cold-end corrosion at 130 °C where a gas boiler is safe.

The efficiency gain, and its limits

The latent heat is worth having. Natural gas has a lower calorific value of about 36 MJ/Nm³ and produces about 1.6 kg of water vapour per normal cubic metre, carrying 3.9 MJ of latent heat, nearly 11% of the fuel’s energy. A condenser cooling the gas to 40 °C recovers most of it; in practice a condensing boiler gains 4-6 points, because the return water limits how far the gas can be cooled and some latent heat leaves with the saturated gas.

The limit is the heat sink. To condense, the gas must be cooled below its dew point, which means the water or air on the other side must be colder than 55 °C. A boiler with 105 °C deaerated feedwater cannot condense in its economiser at all; the feed is hotter than the dew point. That is why condensing economisers are fitted to boilers with low return water temperatures, or to preheat cold make-up water, or to heat a pool or a district heating return. Without a cold sink, a condensing boiler runs in non-condensing mode and its extra surface earns nothing.

The marginal gain falls sharply with surface: a condenser sized for a 15 K approach recovers most of what one twice the size would, and the extra surface is better spent on the economiser.

Materials and cold-end design

Where condensation is intended, the material must tolerate weak acid continuously. ND steel, a low-alloy steel with copper and chromium, is the standard for economiser fins and tubes in condensing service; stainless steel 316L is used for the condenser shell, the drains and the fittings, and plastic or coated steel for the flue downstream of the condenser. Aluminium fins are unacceptable, and ordinary carbon steel lasts a season or two.

Where condensation is not intended, the design must keep the metal above the acid dew point with a margin. The usual rule is a cold-end metal temperature at least 10-15 K above the acid dew point, which for a 1% sulphur fuel means keeping the last surface above 155-165 °C. That is achieved by bypassing part of the feedwater around the economiser, by recirculating feedwater, or by using a steam air preheater rather than a gas-to-air one at low load.

The failure mode of a bypass control is that it is set once and never checked. A boiler that ran at 70% load in winter, with the bypass open to keep the stack at 170 °C, runs at 40% load in summer with the same bypass position and a stack at 120 °C. The cold end condenses, the fins corrode, and the first sign is a plume and a puddle under the economiser. The bypass should be controlled on cold-end metal temperature, not on a fixed valve position.

The signs, and what they cost

Acid corrosion of the cold end is recognisable. The condensate is yellowish with a pH of 2-4, etches concrete and kills grass where it drains. Fins and tubes lose thickness at the gas inlet face, where the metal is coldest, and the stack shows rust streaks at the base and around the test ports. The cost is not only the economiser: acid condensate running back into the boiler carries iron and sulphate into the feedwater, and a leaking tube makes a wet, corrosive slurry that attacks the stack and the fan.

Fuel Sulphur content Acid dew point Minimum cold-end metal
Natural gas Negligible No acid point; water 55-60 °C Above water dew point or condensing design
Light oil 0.1-0.3% 120-135 °C 140 °C
Heavy fuel oil 1-2% 140-155 °C 165 °C
Coal 0.5-2% 130-155 °C 160 °C
Biomass, straw 0.1-0.3% plus chloride 90-130 °C 140 °C, chloride-resistant
Biomass, clean wood Below 0.1% Water 60-65 °C 110 °C

Designing for the right one

The first decision is whether the plant has a cold sink below 50 °C. If it does, a condensing economiser or a separate condenser is worth the material cost and will recover 4-6 points. If it does not, the tail-end surface should be designed as a non-condensing economiser with a cold-end temperature above the acid dew point, and the extra efficiency should come from a larger air preheater or from better burner tuning.

The second decision is drainage. Condensate must leave by gravity through a trapped drain that does not let gas bypass, and be neutralised before it reaches a drain. A condensing boiler makes 1-2 litres per cubic metre of gas, which for a 4 t/h unit is 200-300 litres a day; an undersized drain or a dry trap is a guaranteed corrosion problem. The neutralising trap, the slope and the cleaning access are part of the system.

The third decision is the stack. Below the dew point the gas is saturated and the plume visible, so the stack must be stainless or plastic-lined, insulated and drained at the base. Above it, ordinary steel is fine. A condensing economiser on a mild steel stack is the mistake that rusts the stack within two years and draws a complaint about the plume.

Condensation is neither good nor bad in itself. It is a phase change that releases heat and creates acid, and the design either captures the first and manages the second, or it does neither. The temperature at the cold end is the single number that decides which.